抄録
A new processing method for solidifying calcium carbonate (CaCO3) powder has been developed using hydrothermal hot-pressing technique. The solidification of calcium carbonate was achieved via vaterite/aragonite-calcite wet transformation under the conditions of the low temperature range of 50≈175°C within short period of below 4.0 h. The tensile strength of the solidified CaCO3 body based on aragonite reached approximately 8.0 MPa. Moreover, the tensile strength of the body could be enhanced by the addition of Chitosan.
本文言語 | English |
---|---|
ページ | 694-700 |
ページ数 | 7 |
出版ステータス | Published - 1996 12 1 |
外部発表 | はい |
イベント | Proceedings of the 1996 4th Materials Engineering Conference. Part 1 (of 2) - Washington, DC, USA 継続期間: 1996 11 10 → 1996 11 14 |
Other
Other | Proceedings of the 1996 4th Materials Engineering Conference. Part 1 (of 2) |
---|---|
City | Washington, DC, USA |
Period | 96/11/10 → 96/11/14 |
ASJC Scopus subject areas
- Building and Construction